The highest regioregularity P3HT (M104, RR = 96.3%) produces highly crystalline films and is recommended for OFETs, nanofibril formation and fast drying OPVs at the thin interference peak (90 nm). However, the exceptionally high regioregularity of this P3HT means that gelling and surface roughness can be an issue for slow-drying thick-film OPVs (>200 nm). Lower molecular weight and regioregularity P3HT is recommended for inkjet and other large area or slow drying deposition techniques where gelling/aggregation and surface roughness need to be avoided.

A fabrication report with mobility measurements of 0.12 cm2/Vs for M104 can be found below.

All the P3HT below is highly soluble (50 mg/ml) in chlorinated solvents such as chloroform, chlorobenzene, dichlorobenzene and trichlorobenzene. The intermediate and lower molecular weight P3HT materials are recommended for use with non-chlorinated solvents such as xylene, toluene and THF due to their increased solubility.

CAS number: 104934-50-1

 

Usage Details

Mobility Measurements for M104 - Fabrication Routine

A full fabrication report can be downloaded here.

Field effect mobilities in excess of 0.12 cm2/Vs are recorded using M104 when the active layer is dispensed on OTS-treated silicon oxide dielectric by static spin coating from an optimized high/low boiling point solvent mix.

High hole mobility in conjunction with good solubility and partial air stability make regioregular P3HT a reference material of choice for both fundamental and applied research in organic electronic, physics and chemistry. As one of the most well-studied organic semiconductor, P3HT is often acknowledge to be one of the benchmark against which any new p-type or donor conjugate molecule should be compared and evaluated.

Mobility has previously been found to be positively correlated with increasing region-regularity, slow drying time (achieved using high boiling point solvent), lowering of the surface energy, and molecular weight in excess of 50 kD. These conditions favour p-p stacking parallels to the OFET substrate, which in turn results in improved charge transport across the transistor channel [1-13].

 

Substrate size20 x 15 mm
Gate conductivity1-30 O·cm (Boron doped)
Silicon oxide thickness300 nm
Device per substratesFive, common gate
Channel length30 µm
Channel width1000 µm

 

The active layer solution preparation, spin coating, substrate annealing and measurements are performed in a glove box under a nitrogen atmosphere (H2O <0.1 PPM; O2 < 5/8 PPM).

For generic details on the fabrication of OPV devices, please see our written guide and video demonstration.

Active Layer Preparation

High-Regioregular and high molecular weight RR-P3HT (M104) (RR = 96.3%, Mw = 77,500, Mn = 38,700) is dissolved in a mix of high and low boiling point solvent in order to exploit the beneficial effect of long drying time and increase the wettability of low energy surface, respectively.

  • 5 mg/ml of M104 dissolved in anhydrous Chloroform:Trichlorobenzene (99:1) mix;
  • Vial is placed on hot plate (70°C) with a stirrer bar for 30 minutes;
  • Solution cooled down at room temperature and then filtered with a 0.45 µm PTFE filter;
  • Solution stored overnight on a hot plate at 30°C to prevent excessive aggregation of the P3HT molecules.

Substrate Cleaning

  • Substrates loaded on to substrate rack (to keep them in upright position);
  • Sonicated in hot Hellmanex solution (1%) for five minutes;
  • Rinsed twice in hot water;
  • Sonicated in warm Isopropyl alcohol (70°C) for five minutes;
  • Rinsed twice in cold DI water;
  • Substrates stored in DI water.

Thermal Deposition of Electrodes and Contact Pads

  • Done on Edwards 306 Thermal coater in clean room condition;
  • Substrates are blown dry and loaded in a low density evaporation stack with a low density shadow mask to pattern the desired features;
  • Secondary mask is added to selectively evaporate the gate and drain/source pads;
  • Vacuum chamber pumped down to a vacuum pressure of 5 x 10-6 mbar;
  • Chromium adhesion layer: 5 nm, rate 0.05 nm/s;
  • Aluminium: 80 nm, rate: 0.4 nm/s;
  • Changed secondary mask to deposit electrodes (FET channels);
  • Vacuum: 2-3 x 10-6 mbar;
  • Chromium adhesion layer: 1 nm, rate 0.05 nm/s;
  • Gold: 40 nm; rate 0.05 nm/s.

PFBT Treatment for Au Electrodes (Laminar flow)

  • Oxygen plasma treatment, 30 seconds at 100 W;
  • Substrates immersed in 2.5 mMol/l solution of PFBT in isopropyl alcohol at room temperature;
  • Substrates rinsed twice in pure isopropyl alcohol;
  • Substrates are blown with nitrogen gun.

OTS Treatment for SiO2 Dielectric (Laminar flow)

  • 200 µl solution of pure OTS in cyclohexane, anhydrous grade, prepared in glove box so to obtain a final concentration of 1 mMol/l;
  • Trough filled with 60 ml of cyclohexane, HPLC grade, in laminar flow;
  • Previously prepared OTS solution quickly added to the cyclohexane and mixed with a pipette tip;
  • Substrate (pre-loaded on a substrate rack) immersed in the trough;
  • Trough topped up with extra 3 ml cyclohexane and closed with a glass lid. The final solution (63 ml) contain OTS at a concentration of 1 mMol/l;
  • Substrates kept for 18 minutes in the OTS solution;
  • Substrates removed from the OTS solution, quickly rinsed twice in clean Cyclohexane, and then are blown dry with nitrogen gun.

Contact Angle Assessment

The water-drop test on the treated silicon is a quick test to qualitatively assess the effect of the OTS on the silicon substrates, see Fig. 3. Note that quantitative assessment has previously shown this routine to produce contact angles of 110°C and this test is used as a quick reference to ensure fabrication has functioned correctly.

P3HT (M104) spin coating (glove box)

  • 30 µl of Organic Semi-Conductor (OSC) solution delivered on the middle of the substrate and then spin coated at 1000 rpm for 10 s followed by 60 s at 2000 rpm;
  • Cotton swab soaked in chlorobenzene to thoroughly wipe clean the contact pads and the rest of the substrates with the exception of the area around the channel;
  • High precision cotton swab to clean between devices to avoid cross-talking and reduce leakage;
  • Substrates annealed at 90°C for 30 minutes;
  • Cooled down for ten minutes;
  • Five devices per substrate automatically characterised using Ossila FACT1 in glove box, see Fig 4;
  • Second annealing at 120°C for 20 minutes, slow cooling down at room temperature and measurement;
  • Annealing at 150°C for 20 minutes, slow cooling down at room temperature and measurement.

 

想了解更詳細(xì)的產(chǎn)品信息,填寫下表直接與我們聯(lián)系:

留言框

  • 產(chǎn)品:

  • 您的單位:

  • 您的姓名:

  • 聯(lián)系電話:

  • 常用郵箱:

  • 省份:

  • 詳細(xì)地址:

  • 補充說明:

  • 驗證碼:

    請輸入計算結(jié)果(填寫阿拉伯?dāng)?shù)字),如:三加四=7
深圳市澤拓生物科技有限公司 專業(yè)提供:大小鼠解剖器械包,瑞士Sipel真空泵,美國EMS電鏡耗材
深圳市澤拓生物科技有限公司版權(quán)所有   |   技術(shù)支持:化工儀器網(wǎng)
聯(lián)系電話:0755-23003036   傳真:0755-23003036-807 GoogleSitemap 備案號:粵ICP備17105262號  管理登陸
在線客服
久久久久久久久av毛片| 亚洲无人区天空码头IV| 日本xxxxx18学生老师| 黑人猛干亚洲女久久不见网| 国产做爰全免费的视频软件| 五十路熟妇高熟无码| 国产亚洲av日韩精品熟女| 无码日本电影一区二区网站| 亚洲A片成人片在线观看| 免费网站看v片在线香蕉| 制服丝袜电影| aaa毛片一区二区三区| 亚洲国产成人毛片做暖暖| 2021精品人妻少妇网站| 91大神在线精品免费福利| 麻豆国产av超爽剧情系列| 亚洲男人的天堂2021| 欧美国产日韩高清在线综合| 日韩亚洲欧美一区二区三区| 三年成全免费看全视频| 粉嫩xb粉嫩xb粉嫩xb| 亚洲综合18禁| 亚洲国产色婷婷久久精品| 干一夜综合| 深夜a级毛片免费无码| 欧美精品videosex极品| 色噜噜一区二区三区| 天堂中文在线最新版地址| 999久久久一区二区三区| 欧美日韩在线精品一二区| 国产免费无码又爽又激情| 白嫩丰满大屁股bbbbb肥波婆| 日韩福利片午夜在线观看| 青青草激情视频在线播放| 国产成人91亚洲精品无| 亚洲国产精品成人精品小说| 自拍性旺盛老熟女| 日本淫秽色视频在线播放| 强壮公弄得我次次高潮小说| g0g0全球高清大胆人休艺术网| 午夜男人网站|